Table of Contents
FN-0208 is a nickel-strengthened powder metallurgy alloy containing 2% nickel and 0.8% carbon, offering an optimized balance between mechanical strength and manufacturing cost. With tensile strengths of 420-480 MPa in the as-sintered condition and 650-750 MPa after heat treatment, FN-0208 delivers 35-45% higher strength than plain carbon PM steels while costing 40-50% less than higher-nickel alloys like FN-0405.
This mid-tier PM alloy has become the industry standard for automotive transmission components, lawnmower gears, and light-duty power tool parts where moderate mechanical loads require strength improvements over plain carbon steels but don't justify the expense of 4% nickel alloys.
What is FN-0208 Powder Metallurgy Alloy?
FN-0208 is designated under MPIF Standard 35 (Metal Powder Industries Federation) as a pre-alloyed nickel-carbon steel powder specifically formulated for structural applications requiring enhanced mechanical properties. Browse all MPIF Standard 35 material families to see how FN-0208 fits within the broader PM alloy system.
FN-0208 Chemical Composition
| Element | Weight % | Function |
|---|---|---|
| Nickel (Ni) | 2.0% | Solid solution strengthening, hardenability improvement |
| Carbon (C) | 0.6-0.9% (typically 0.8%) | Strength, hardness, heat treatment response |
| Iron (Fe) | Balance (~97%) | Base matrix material |
| Molybdenum (Mo) | Optional: 0.5-1.0% | Additional hardenability (FN-0208-Mo variant) |
The 2% nickel content provides the critical balance:
- Sufficient strengthening: 35-45% strength increase over plain carbon steels
- Cost effectiveness: Uses 50% less nickel than FN-0405 alloys
- Heat treatment response: Enables through-hardening to HRC 30-38
- Dimensional stability: Lower distortion than higher-nickel alternatives
FN-0208 Mechanical Properties
As-Sintered Properties (Standard Processing)
| Property | Value | Test Standard |
|---|---|---|
| Tensile Strength | 420-480 MPa (61-70 ksi) | MPIF 10 |
| Yield Strength (0.2% offset) | 300-350 MPa (43-51 ksi) | MPIF 10 |
| Elongation | 1.5-2.5% | MPIF 10 |
| Hardness | HRB 75-85 (HRC 0-8 equivalent) | ASTM E18 |
| Impact Energy (Unnotched) | 18-24 J (13-18 ft-lbs) | MPIF 40 |
| Fatigue Strength (10⁷ cycles) | 180-210 MPa | MPIF 56 |
| Density | 7.0-7.2 g/cm³ | MPIF 42 |
Processing Conditions: Sintered at 1120°C (2050°F) in dissociated ammonia atmosphere for 20-30 minutes, typical density 91-93% of theoretical.
Heat-Treated Properties
Through-Hardening (Oil Quench + Tempering):
- Austenitizing: 845-870°C (1550-1600°F), 20-30 minutes
- Quenching: Fast oil or intensive quench
- Tempering: 175-205°C (350-400°F), 1 hour
| Property | Heat-Treated Value | Improvement vs As-Sintered |
|---|---|---|
| Tensile Strength | 650-750 MPa (94-109 ksi) | +55-60% |
| Yield Strength | 550-650 MPa (80-94 ksi) | +83-86% |
| Hardness | HRC 30-38 (HRB 100+ equivalent) | +300-375% |
| Fatigue Strength | 280-320 MPa | +55-60% |
**Case Hardening (Carburizing):**
- Surface Hardness: HRC 55-60 (case depth 0.5-1.0 mm)
- Core Hardness: HRC 20-28
- Fatigue Strength: 320-380 MPa (significant improvement in bending/contact fatigue)
💡 Engineering Note: FN-0208 offers 75-80% of FN-0405's heat-treated strength at 60% of the material cost, making it the preferred choice for applications with tensile stress <700 MPa.
Comparison: FN-0208 vs Other PM Alloys
| Material | Tensile Strength (As-Sintered) | Tensile Strength (Heat-Treated) | Relative Cost | Best Applications |
|---|---|---|---|---|
| FC-0000 (Pure Iron) | 210-250 MPa | 280-340 MPa | 1.0x | Magnetic components, low-load |
| FC-0208 (0.8% C) | 320-380 MPa | 520-620 MPa | 1.1x | Moderate load, cost-sensitive |
| FN-0208 (2% Ni) | 420-480 MPa | 650-750 MPa | 1.5x | Automotive gears, clutches |
| FN-0405 (4% Ni) | 550-620 MPa | 850-950 MPa | 2.2x | Heavy-duty transmissions |
| FN-0408 (8% Ni) | 620-700 MPa | 1000-1100 MPa | 3.8x | Extreme load applications |
Selection Criteria:
- Choose FC-0208 if: Loads <400 MPa, cost is critical, no impact loads
- Choose FN-0208 if: Loads 400-700 MPa, moderate impact, standard automotive
- Choose FN-0405 if: Loads 700-900 MPa, high impact, heavy-duty automotive
- Choose FN-0408 if: Loads >900 MPa, extreme impact, aerospace/defense
FN-0208 Manufacturing Process
1. Powder Metallurgy Production Steps
Powder Characteristics:
- Particle Size: -100/+325 mesh (45-150 μm)
- Apparent Density: 2.8-3.2 g/cm³
- Flow Rate: 25-30 s/50g (Hall flowmeter)
- Pre-alloying: Nickel fully alloyed during atomization (ensures homogeneity)
Compaction:
- Pressure: 550-700 MPa (40-50 tsi)
- **Green Density**: 6.8-7.0 g/cm³
- **Green Strength**: 15-20 MPa (sufficient for handling)
- Lubricant: 0.75% zinc stearate (removed during dewax cycle)
Sintering:
- Dewax Zone: 400-600°C, 15 minutes (lubricant removal)
- Sintering Temperature: 1120-1135°C (2050-2075°F)
- Atmosphere: Dissociated ammonia (75% H₂, 25% N₂) or N₂-H₂ blend
- Time at Temperature: 20-30 minutes
- Cooling: Slow cool to 550°C, then accelerated cooling
Dimensional Control:
- Sintered Growth: +0.1% to +0.3% (depending on density)
- Tolerance: ±0.05-0.10 mm typical for as-sintered dimensions
- Sizing Operations: Can achieve ±0.02 mm on critical features
2. Secondary Operations
Machining:
- As-Sintered Machinability: Good (comparable to 1020 carbon steel)
- Heat-Treated Machinability: Moderate (HRC 30-38 range)
- Recommended: Pre-machine before heat treatment when possible
**Steam Treatment (Optional):**
- Improves surface hardness to HRB 90-95
- Enhances wear resistance by forming Fe₃O₄ layer
- Seals surface porosity, improves corrosion resistance
Surface Densification:
- Rolling/Sizing: Can achieve 7.3-7.4 g/cm³ surface density
- Shot Peening: Improves fatigue strength by 15-25%
Primary Applications of FN-0208
1. Automotive Transmission Components
Transmission Gears (Light-Medium Duty):
- Applications: Manual transmission synchronizer gears, planetary carrier gears (light trucks), overdrive gears
- Typical Design: 25-60 mm diameter, 2.0-2.5 module, 20-40 teeth
- Performance: 350-500 Nm torque capacity, 2-3 million cycle life
- Heat Treatment: Through-harden to HRC 32-36 or carburize case to HRC 58-60
- Cost Advantage: 45-55% lower than machined FN-0405
Clutch Components:
- Clutch hubs, pressure plate fingers, sprocket carriers
- Requires dimensional stability (±0.03 mm on critical diameters)
- As-sintered condition often sufficient (HRB 80-85)
2. Lawn & Garden Equipment
Lawnmower Gears:
- Drive Gears: Transmission between engine and blade/wheels
- Starter Gears: Recoil starter mechanisms
- Performance Requirements: 15-25 Nm torque, impact-resistant
- Heat Treatment: Through-harden to HRC 28-32 (resists impact from stones)
Small Engine Components:
- Crankshaft gears, camshaft gears, oil pump gears
- Typical density: 7.1-7.2 g/cm³ (reduces oil porosity)
3. Power Tools (Light-Duty Applications)
Drill & Driver Gears:
- Planetary Gearbox: Sun gears, planet gears (12-18V cordless tools)
- Load Conditions: Intermittent duty, 5-15 Nm peak torque
- Material Selection: FN-0208 as-sintered (HRB 80) sufficient for homeowner-grade
- Note: Professional-grade tools often upgrade to FN-0405
Impact Mechanism Components:
- Hammer anvils (light-duty impact drivers)
- Requires case hardening (HRC 58-60 surface, HRC 25-30 core)
4. Industrial Machinery (Light-Load Applications)
Conveyor System Gears:
- Material handling, packaging equipment gears
- Low-speed, low-shock applications (<50 rpm, <100 Nm)
Pump Components:
- Gear pump gears (hydraulic, water, light oil)
- Requires steam treatment for corrosion resistance
- Density >7.2 g/cm³ to minimize fluid infiltration
FN-0208 Heat Treatment Guidelines
Through-Hardening Process
Recommended Cycle:
- Preheat (optional for complex shapes): 650°C, 10 minutes
- Austenitizing: 855°C ±10°C (1570°F), hold 25 minutes
- Quenching: Fast oil (60-80°C) with agitation
- Tempering: 190°C (375°F), 60 minutes
Expected Results:
- Core hardness: HRC 32-36
- Distortion: <0.15 mm on 50 mm diameter gear
- Tensile strength: 690-740 MPa
Critical Parameters:
- Carbon Potential: Maintain neutral atmosphere (0.75-0.85% C equivalent)
- Quench Delay: <5 seconds from furnace to quench tank
- Tempering Temperature: Every 15°C increase reduces hardness by ~2 HRC points
Case Hardening (Carburizing)
Gas Carburizing Cycle:
- Boost Stage: 925°C, 1.0-1.2% carbon potential, 2-4 hours (target 0.8-1.0 mm case)
- Diffusion Stage: 845°C, 0.8% carbon potential, 30-60 minutes
- Direct Quench: Oil quench from 845°C
- Temper: 175°C, 90 minutes
Case Properties:
- Effective Case Depth: 0.5-1.0 mm (to HRC 50)
- Surface Hardness: HRC 56-60
- Core Hardness: HRC 20-28
- Surface Carbon: 0.9-1.1%
Carbonitriding Alternative:
- Lower temperature (815-845°C) reduces distortion
- Adds nitrogen for enhanced surface hardness
- Case depth: 0.15-0.40 mm (suitable for wear resistance)
Dimensional Change Management
| Heat Treatment Type | Typical Growth | Distortion (Out-of-Round) |
|---|---|---|
| As-Sintered | 0% (baseline) | N/A |
| Through-Harden + Temper | +0.05% to +0.15% | 0.03-0.08 mm on Ø50 mm |
| Carburize + Quench | +0.10% to +0.25% | 0.08-0.15 mm on Ø50 mm |
| Carbonitriding | +0.05% to +0.12% | 0.04-0.10 mm on Ø50 mm |
Distortion Minimization:
- Use press quenching for tight-tolerance gears
- Orient part for uniform cooling (suspend vertically)
- Temper immediately after quenching (<1 hour delay)
Design Considerations for FN-0208 Components
1. Density Requirements
Target Density Selection:
| Application Type | Minimum Density | Rationale |
|---|---|---|
| Structural Gears (Dry) | 7.0 g/cm³ | 90-91% density provides adequate strength |
| Lubricated Gears | 7.1 g/cm³ | Reduces oil absorption, improves fatigue |
| Hydraulic Components | 7.2 g/cm³ | Minimizes fluid infiltration |
| High-Stress Parts | 7.3 g/cm³ (repress) | Approaches wrought properties |
2. Porosity Management
Oil Impregnation (for bearing surfaces):
- Standard FN-0208 at 7.0 g/cm³: 10-12% interconnected porosity
- Can absorb 8-10 vol% oil for self-lubrication
- Oil retention: SAE 30 motor oil typically used
Surface Sealing (when required):
- Steam treatment: Creates Fe₃O₄ layer, seals <5 μm pores
- Resin impregnation: Fills porosity with thermosetting polymer
- Surface densification: Rolling/sizing operations
3. Geometry Limitations
Maximum Wall Thickness:
- Uniform Compaction: 25-30 mm wall sections
- Complex Shapes: Length-to-diameter ratio <3:1
- Thin Walls: Minimum 2.0 mm (thinner walls risk cracking)
Feature Tolerances:
- As-Sintered: ±0.08-0.15 mm on non-critical dimensions
- Sized: ±0.02-0.05 mm on critical diameters/faces
- Heat-Treated: Add +0.05-0.10 mm growth allowance
Draft Angles:
- Minimum 0.5° draft for compaction tooling removal
- Straight walls possible with special tooling (adds cost)
Cost Analysis: FN-0208 vs Alternatives
Material & Processing Costs
| Process | Material Cost ($/kg) | Processing Cost ($/part)* | Total Cost Index |
|---|---|---|---|
| FC-0208 PM | $2.80 | $0.85 | 1.0x (baseline) |
| FN-0208 PM | $4.20 | $0.85 | 1.4x |
| FN-0405 PM | $7.00 | $0.85 | 2.2x |
| Machined 8620 | $3.50 | $4.50 | 3.9x |
| Machined 4320 | $5.80 | $4.50 | 4.7x |
*Typical automotive gear, 50g part weight, production volume >100,000 units/year
Break-Even Analysis: FN-0208 vs Machining
Example: Manual transmission synchronizer gear, Ø40mm × 12mm thick
Tooling Investment:
- PM Tooling (die set): $12,000-18,000
- Machining Fixtures: $3,000-5,000
Per-Part Economics (50,000 units/year):
| Cost Element | FN-0208 PM | Machined 8620 | Savings |
|---|---|---|---|
| Material | $0.21 | $0.45 | $0.24 |
| Compaction | $0.12 | — | — |
| Sintering | $0.18 | — | — |
| Machining | $0.15 (secondary) | $2.80 | $2.65 |
| Heat Treatment | $0.22 | $0.35 | $0.13 |
| Total per Part | $0.88 | $3.60 | $2.72 |
| Annual Savings | — | — | $136,000 |
| Payback Period | 1.2 months | — | — |
When to Choose FN-0208 PM:
- Production volume >5,000 units (tooling amortization)
- Part geometry suited to compaction (no deep undercuts)
- Tolerances achievable with sizing (<±0.03 mm critical features)
- Material properties meet mechanical requirements
Case Study: Lawnmower Transmission Gear Conversion
Project Background
Client: Major outdoor power equipment manufacturer (residential lawnmowers) Component: Main transmission drive gear (manual push mowers) Original Design: Machined 1045 carbon steel, through-hardened to HRC 28-32 Challenge: Reduce production costs while maintaining 1,500-hour durability requirement
Original Design (Machined)
Specifications:
- Material: AISI 1045 carbon steel bar stock
- Geometry: Ø38 mm, 15 mm face width, 24 teeth (2.5 module)
- Processing: CNC turning, hobbing, heat treat (through-harden), finish grinding
- Properties: HRC 30 ±2, tensile strength ~620 MPa
- Production Cost: $3.85/part at 80,000 units/year
Performance:
- Torque Transmission: 22 Nm continuous, 45 Nm peak (blade impact)
- Durability: 2,200-hour average life (exceeds requirement)
- Failure Mode: Tooth wear after 2,000+ hours (end of product life)
Redesign with FN-0208 PM
Material Selection Rationale:
- FN-0208 chosen over FC-0208 for improved impact resistance (stones, branch impacts)
- Through-hardening to HRC 32-35 provides equivalent hardness to original
- Nickel content enhances hardenability (uniform core hardness)
Design Modifications:
- Geometry: Same tooth profile, increased face width 15 mm → 17 mm (compensates for slightly lower fatigue strength)
- Density Target: 7.1 g/cm³ (91.5% density)
- Processing: Compaction → Sinter → Heat treat (through-harden) → Sizing on bore/face
Manufacturing Process:
- Compaction: 650 MPa, achieves 6.95 g/cm³ green density
- Sintering: 1120°C, 25 minutes, N₂-H₂ atmosphere
- Heat Treatment: Austenitize 855°C, oil quench, temper 190°C
- Sizing: Repress bore and face for ±0.03 mm tolerance
- Inspection: 100% hardness test (HRC 31-35 acceptable range)
Results
Performance Validation:
- Accelerated Life Testing: 10 gears tested to 2,500 hours (no failures)
- Field Testing: 500 mowers monitored over 1 season (average 85 hours use)
- Failure Analysis: No premature gear failures observed
- Durability: Estimated 2,000-hour life (matches original, exceeds requirement)
Cost Reduction:
| Cost Category | Original (Machined) | FN-0208 PM | Savings |
|---|---|---|---|
| Material | $0.58 | $0.16 | $0.42 |
| Machining | $2.45 | $0.18 | $2.27 |
| Heat Treatment | $0.52 | $0.24 | $0.28 |
| Grinding | $0.30 | — | $0.30 |
| Total Cost | $3.85 | $0.58 | $3.27 |
| Annual Savings | — | — | $261,600 |
Additional Benefits:
- Weight Reduction: 15% lighter (porosity), reduces inertia loads
- Quieter Operation: PM material dampens vibration, reduces gear noise by 2-3 dB(A)
- Simpler Supply Chain: Single supplier (vs machining + heat treat subcontractors)
Tooling Investment:
- Die set cost: $14,500
- Payback period: 3.4 weeks of production
- Expected die life: 1.5 million cycles (18+ years production)
Lessons Learned
- Design for PM: Increasing face width 13% compensated for 10% lower fatigue strength vs wrought steel
- Heat Treatment Validation: Trial batches confirmed consistent HRC 32-35 achievable across production
- Sizing Critical: Bore and face required sizing to meet assembly tolerances (±0.03 mm)
- Density Matters: 7.1 g/cm³ minimum density necessary for impact resistance (stone strikes)
Quality Control & Testing for FN-0208 Parts
Incoming Powder Inspection
| Test | Specification | Frequency |
|---|---|---|
| Apparent Density | 2.8-3.2 g/cm³ | Every lot |
| Flow Rate | 25-30 s/50g | Every lot |
| Particle Size Distribution | -100/+325 mesh (90%) | Every 3rd lot |
| Chemistry | Ni: 1.9-2.1%, C: 0.7-0.9% | Certificate of Analysis |
In-Process Controls
Green Part (Post-Compaction):
- Dimensions: Measure critical features (±0.10 mm green tolerance)
- Green Density: 6.8-7.0 g/cm³ (weigh + measure volume)
- Green Strength: >15 MPa (ensure handling integrity)
Sintered Part (Post-Sinter):
- Dimensions: ±0.08 mm on critical features
- Sintered Density: 7.0-7.2 g/cm³ (Archimedes method per MPIF 42)
- Hardness: HRB 75-85 (as-sintered baseline)
- Microstructure: Pearlite + ferrite + <12% porosity
Heat-Treated Part:
- Hardness Mapping: Test 3 locations (surface, mid-radius, core) to verify HRC 32-36 range
- Dimensions: Check for distortion (<0.10 mm out-of-round on gears)
- Microstructure: Tempered martensite, uniform case depth (if carburized)
Final Inspection & Testing
Destructive Testing (sample basis):
- Tensile Testing: MPIF 10 standard (verify ≥650 MPa heat-treated)
- Impact Testing: Unnotched Charpy (verify ≥25 J)
- Fatigue Testing: Rotating beam at 10⁷ cycles (verify ≥280 MPa endurance limit)
Non-Destructive Testing (100% or sampling):
- Dimensional Inspection: CMM or gauging per drawing
- Hardness Testing: Rockwell C scale (HRC 32-36 acceptance)
- Visual Inspection: Surface defects, cracks, sink marks
- Magnetic Particle Inspection: Critical automotive parts (crack detection)
Troubleshooting Common FN-0208 Issues
Problem 1: Low Hardness After Heat Treatment (HRC <30)
Possible Causes:
- Insufficient austenitizing temperature or time
- Slow quench rate (oil contamination, insufficient agitation)
- Decarburization during sintering or heat treatment
Solutions:
- Verify furnace temperature calibration (±5°C accuracy)
- Check quench oil condition (replace if >10% water contamination)
- Use protective atmosphere during austenitizing (endothermic gas or vacuum)
- Consider carbonitriding to add surface carbon
Problem 2: Excessive Distortion After Quenching
Possible Causes:
- Non-uniform part temperature during quenching
- Asymmetric part geometry or density variations
- Retained austenite transformation
Solutions:
- Use press quenching for tight-tolerance parts
- Orient parts vertically in quench tank (uniform cooling)
- Add refrigeration treatment (-80°C, 2 hours) to transform retained austenite
- Design symmetrical geometry where possible
Problem 3: Premature Gear Tooth Failure
Possible Causes:
- Insufficient case depth (carburized parts)
- Surface porosity allowing stress concentration
- Improper gear lubrication
Solutions:
- Increase carburizing time for deeper case (0.8-1.0 mm effective depth)
- Increase density to 7.2 g/cm³ minimum (reduces surface porosity)
- Apply steam treatment to seal surface porosity
- Verify lubricant viscosity and application rate
Problem 4: Poor Machinability (Excessive Tool Wear)
Possible Causes:
- Over-hardening (HRC >38 in areas to be machined)
- Abrasive porosity causing tool wear
- Incorrect cutting parameters
Solutions:
- Machine before heat treatment (preferred solution)
- Reduce hardness to HRC 30-32 if post-heat-treat machining required
- Use sharp carbide tooling with positive rake angles
- Apply cutting fluid generously (flood coolant)
Frequently Asked Questions (FAQ)
1. What is the main advantage of FN-0208 over plain carbon PM steels?
FN-0208 provides 35-45% higher tensile strength (420-480 MPa as-sintered vs 320-380 MPa for FC-0208) due to nickel's solid solution strengthening effect. This allows use in moderate-load applications like automotive transmission gears and lawnmower components where plain carbon steels lack sufficient strength. The 2% nickel content also significantly improves hardenability, enabling through-hardening to HRC 32-36 with uniform core properties.
2. When should I choose FN-0208 instead of FN-0405?
Choose FN-0208 when:
- Design stress levels are <700 MPa (FN-0208 heat-treated: 650-750 MPa)
- Cost is a significant factor (FN-0208 is 40-50% less expensive)
- Application involves light-to-moderate mechanical loads
- Impact resistance requirements are moderate (not severe shock loads)
Choose FN-0405 when:
- Design stress levels exceed 750 MPa
- Heavy-duty automotive transmission (truck, bus)
- High impact loads (severe shock, cyclic overload)
- Maximum fatigue life is critical
3. Can FN-0208 be welded?
FN-0208 PM parts can be welded, but special precautions are required:
- Porosity Sealing: Apply resin impregnation to seal pores (prevents weld contamination)
- Preheat: Preheat to 200-250°C to reduce thermal shock
- Welding Method: TIG or MIG preferred (better control than stick welding)
- Post-Weld Heat Treatment: Stress relieve at 590-620°C for 1 hour
Note: Welding PM parts is generally avoided due to porosity. Consider redesigning as multiple components joined mechanically if welding seems necessary.
4. What density should I specify for FN-0208 gears?
Recommended densities by application:
- Light-Duty Gears (lawnmowers, small engines): 7.0-7.1 g/cm³
- Automotive Transmission Gears (manual, light trucks): 7.1-7.2 g/cm³
- High-Stress Gears (power tools, industrial): 7.2-7.3 g/cm³
Higher density improves fatigue strength but increases cost (higher compaction pressure, potential secondary densification). Balance mechanical requirements against cost targets.
5. How does FN-0208 compare to wrought 4320 nickel steel?
Strength Comparison:
- FN-0208 Heat-Treated: 650-750 MPa tensile, HRC 32-36
- Wrought 4320 Heat-Treated: 1000-1200 MPa tensile, HRC 38-42
Cost Comparison:
- FN-0208 PM: 40-60% lower cost (near-net-shape, minimal machining)
- Wrought 4320: Expensive material + extensive machining
When to Use Each:
- Use FN-0208 for moderate loads, high-volume production, cost-sensitive
- Use 4320 for extreme loads, critical safety, low-volume/prototype
6. What is the typical lead time for FN-0208 PM tooling?
Die Set Fabrication: 6-10 weeks depending on complexity
- Simple geometry (cylindrical gear): 6-7 weeks
- Complex shapes (multi-level, internal features): 8-10 weeks
Production Sampling: 2-3 weeks after tooling delivery (includes dimensional validation, property testing, heat treatment trials)
Total Time to First Production Parts: 8-13 weeks from design freeze
7. Can FN-0208 be used for self-lubricating bearings?
Yes, FN-0208 can be oil-impregnated for limited self-lubricating applications, but it's not optimal:
- Porosity: 10-12% at 7.0 g/cm³ density (can absorb 8-10 vol% oil)
- Limitation: Higher strength means higher density, less oil capacity vs dedicated bearing materials
- Better Alternative: Iron-graphite materials (FC-0008) designed specifically for self-lubrication (15-20% porosity)
Use FN-0208 for self-lubricating applications only when strength requirements exceed iron-graphite capability (~250 MPa limit).
8. What tolerances can be achieved with FN-0208 PM?
As-Sintered:
- General dimensions: ±0.10-0.15 mm
- Critical dimensions (sized): ±0.02-0.05 mm
- Flatness: 0.05-0.10 mm over 50 mm span
Heat-Treated:
- Add +0.05-0.10 mm growth allowance
- Distortion (out-of-round): 0.03-0.10 mm typical on gears
- Tight tolerances may require post-heat-treat grinding
Recommended Design Practice: Specify ±0.08 mm on non-critical dimensions, ±0.03 mm on critical features (with sizing operation).
Get Expert FN-0208 Manufacturing Support
Need guidance on material selection, heat treatment optimization, or cost analysis for your FN-0208 components? SinterWorks PM specializes in nickel-alloy powder metallurgy with 16+ years of automotive and industrial gear manufacturing experience.
What we offer: ✅ FN-0208 vs FN-0405 cost-benefit analysis for your specific application ✅ Heat treatment process development (through-hardening, carburizing, carbonitriding) ✅ Design-for-manufacturing review (optimize for PM production) ✅ Prototype tooling and pre-production sampling ✅ Full metallurgical lab testing (tensile, fatigue, hardness mapping)
Contact our engineering team for a free material selection consultation: [Request FN-0208 Technical Support →]
Standards & References
Grade designations and material property data on this page follow published powder metallurgy industry standards. Current editions are available from the publishers:
- MPIF Standard 35 — Materials Standards for PM Structural Parts — Metal Powder Industries Federation (MPIF)
- ASTM International — metal powder and PM material specifications — ASTM International
- ISO 5755 — Sintered metal material: Specifications — ISO
For critical applications, always verify grade data against the current edition of the applicable standard and your part-specific validation requirements.
Expert Review
Yao Qingpu
Powder Metallurgy Manufacturing Expert at SinterWorks PM
Yao Qingpu works with global buyers on powder metallurgy design review, material selection, tolerance planning, cost-down opportunities, and production feasibility. His experience covers PM gears, automotive components, structural parts, and practical DFM support for long-run manufacturing programs.
Related Resources
Use these internal links to keep moving through the most relevant guides, service pages, and technical references for this topic.
FN-0405 High-Nickel Alloy
Compare a stronger higher-nickel PM alternative when impact resistance or fatigue margin needs to increase.
FC-0208 Material Properties
Review a more cost-focused iron-copper PM route when nickel alloy performance is not necessary.
PM Material Grades Overview
Compare FN-0208 against other nickel-steel PM grades in the full MPIF Standard 35 material overview.
Request a Quote
Send your part geometry, target density, and heat-treatment expectations for FN-0208 material guidance and quotation support.