FN-0408 is the premium iron-nickel structural grade in the ferrous PM family defined by MPIF Standard 35 and its ASTM B783 equivalent. The designation reads directly: 04 = approximately 4% nickel, 08 = 0.6-0.9% combined carbon, balance iron. That combination produces the highest as-sintered strength of any standard FN grade — 520-720 MPa tensile at our standard production density window of 7.1-7.4 g/cm³ — and, after quench-and-temper heat treatment, the heat-treated variant FN-0408HT reaches 860-1000 MPa tensile with 40-41 HRC apparent hardness at the densities published in MPIF Standard 35.
Where lower-alloy grades (FC-0205, FN-0205) are cost-optimized for moderate duty, FN-0408 is selected when a component must carry severe, cyclic, or shock loads without a size or weight penalty: premium transmission gears, high-torque power tool gear trains, and extreme-load bearing surfaces. The nickel addition also gives the grade its characteristic mixed microstructure — nickel-rich austenite islands dispersed in a pearlitic steel matrix — which is what sets FN-0408 apart on impact and fatigue behavior, not just on raw tensile strength.
This guide covers FN-0408 composition and standards, as-sintered and heat-treated mechanical properties, processing windows, design guidelines, and a material-to-material comparison against FN-0205, FN-0405, FC-0808, and alternative manufacturing routes. If you are comparing FN-0408 against other PM steels, our FN-0205 vs FN-0405 vs FN-0408 selection guide provides the side-by-side decision logic.
Specifying a high-load gear or bearing component? Upload your drawing for a free FN-0408 feasibility review — material confirmation, density recommendation, and cost comparison within 24 hours.
Get Free FN-0408 Material Consultation →
FN-0408 Composition & Material Standards
Chemical Composition
| Element | Range (%) | Purpose |
|---|---|---|
| Iron (Fe) | Balance | Base metal |
| Nickel (Ni) | 3.0-5.5 | Strength, toughness, hardenability; forms retained austenite islands |
| Carbon (C) | 0.6-0.9 | Combined carbon for pearlite formation and heat-treat response |
| Copper (Cu) | 0.0-2.0 | Residual; optional premix addition |
| Manganese (Mn) | 0.0-0.5 | Deoxidizer, slight hardenability contribution |
Composition per MPIF Standard 35 / ASTM B783. The "08" carbon code (0.6-0.9%) is what physically separates FN-0408 from FN-0405 (0.3-0.6% C): more combined carbon means more pearlite, higher as-sintered hardness, and a full quench-and-temper response.
Material Designation & Standards
- MPIF Standard 35: FN-0408 (as-sintered grades FN-0408-35, -45, -55; heat-treated grades carry the HT suffix)
- ASTM: B783 (ferrous PM structural materials, same designation system)
- ISO: ISO 5755 covers sintered ferrous materials with equivalent designations
- Suffix convention (MPIF): for as-sintered grades the two-digit suffix is the minimum tensile yield strength in ksi; for heat-treated (HT) grades it is the minimum tensile strength in ksi. FN-0408-35 therefore guarantees ≥240 MPa (35 ksi) yield as-sintered, while a heat-treated grade such as FN-0405-155HT guarantees ≥1,070 MPa (155 ksi) ultimate tensile.
Note on the as-sintered condition: all property values in this guide are stated in the as-sintered condition unless explicitly marked HT (heat treated). Heat-treated FN-0408HT delivers substantially higher strength and hardness — see the heat treatment section below.
FN-0408 Key Properties (As-Sintered)
Mechanical Properties — Production Density Window 7.1-7.4 g/cm³
| Property | As-Sintered Value | Units |
|---|---|---|
| Density | 7.1-7.4 | g/cm³ (≈90-94% of wrought steel) |
| Ultimate Tensile Strength | 520-720 | MPa |
| Yield Strength (0.2% offset) | 380-520 | MPa |
| Elongation | 2-4 | % |
| Apparent Hardness | 80-100 | HRB |
| Corrosion Resistance | Low-Moderate | (ferrous PM base; steam treatment or plating recommended) |
| Wear Resistance | Excellent | (heat-treatable to 40+ HRC) |
These are typical as-sintered values across the production density window. The spread is driven primarily by sintered density and combined-carbon control — which is why we specify density explicitly for every FN-0408 program.
Density-Property Ladder
Density is the single biggest lever on FN-0408 strength. Typical as-sintered envelope:
| Density | % of Wrought | Tensile Strength (typical) | Yield Strength (typical) | Hardness (typical) |
|---|---|---|---|---|
| 7.1 g/cm³ | ≈90% | 520-570 MPa | 380-420 MPa | 80-88 HRB |
| 7.25 g/cm³ | ≈92% | 570-650 MPa | 420-470 MPa | 88-95 HRB |
| 7.4 g/cm³ | ≈94% | 650-720 MPa | 470-520 MPa | 95-100 HRB |
Higher density also lifts fatigue and impact values disproportionately — pore structure is the dominant fatigue initiator in PM steels — so premium gear programs usually justify the extra pressing force or a sizing/coining step to hold 7.3+ g/cm³.
MPIF Minimum-Yield Grades (As-Sintered)
For procurement against the standard, MPIF Standard 35 tabulates FN-0408 as-sintered grades by minimum yield strength:
| MPIF Grade | Density Basis | Min. Yield Strength | Elongation (typical) |
|---|---|---|---|
| FN-0408-35 | ≈6.5 g/cm³ | 240 MPa (35 ksi) | ≈1% |
| FN-0408-45 | ≈6.9 g/cm³ | 310 MPa (45 ksi) | ≈1% |
| FN-0408-55 | ≈7.2 g/cm³ | 380 MPa (55 ksi) | ≈1% |
Typical well-sintered production parts exceed these guaranteed minimums — the 520-720 MPa tensile envelope above reflects high-density, controlled-carbon sintering practice rather than the standard's minimum-entry values.
Heat-Treated Condition: FN-0408HT
Quench-and-temper heat treatment transforms FN-0408 into one of the strongest standard PM structural grades. Published MPIF Standard 35 values for FN-0408HT:
| Condition | Density | Tensile Strength | Yield Strength | Elongation | Apparent Hardness |
|---|---|---|---|---|---|
| As-sintered | 7.1-7.4 g/cm³ | 520-720 MPa | 380-520 MPa | 2-4% | 80-100 HRB |
| FN-0408HT (quenched + tempered) | 6.7 g/cm³ | 860 MPa | 740 MPa | <0.5% | 40 HRC |
| FN-0408HT (quenched + tempered) | 7.1 g/cm³ | 1000 MPa | 860 MPa | <0.5% | 41 HRC |
The trade-off is ductility: elongation drops below 1% after through-hardening, so HT parts are designed as wear/strength components rather than impact absorbers. Where quench distortion must be minimized, a higher tempering temperature brings the hardness down to the 35 HRC class in exchange for a more dimensionally stable part — specify the temper window on the drawing rather than accepting a default.
FN-0408 Applications & Industry Use Cases
Premium Gears (Automotive & Power Tools)
FN-0408's home turf. Transmission synchronizer hubs, planetary pinions, and camshaft-drive components use the grade where FN-0205's strength ceiling is reached but machined steel cost cannot be justified. In power tool gear trains (drills, impact drivers, grinders), FN-0408 gears survive repeated shock engagement — the nickel-rich austenite islands arrest crack propagation that would fail a plain carbon-steel PM gear. See our automotive transmission gear and power tool gearbox gear application pages for part-level detail.
Design points for gears:
- Tooth root bending fatigue benefits from 7.3+ g/cm³ density plus shot peening
- Carburize only the tooth flanks/roots when a tough core is required
- Expect ±0.05 mm tolerance after sizing; gear quality up to GB9/DIN 8 with dedicated tooling
Extreme-Load Bearings & Wear Parts
Sintered structural bearings, cam followers, and wear plates run FN-0408 where bronze bushings lack strength and case-hardened wrought steel is over-engineered. As-sintered 80-100 HRB handles abrasive sliding contact; through-hardening to 40 HRC extends life under rolling contact.
Structural Components With Impact Loading
Brackets, lock components, and linkages that see shock loads — seat mechanisms, door checks, striker plates — use as-sintered FN-0408 for its toughness margin over plain iron-carbon grades.
Where FN-0408 Is Not the Right Choice
- Corrosive environments: ferrous PM base with Low-Moderate corrosion resistance. Use 304 stainless PM or 316L, or plan steam treatment/plating.
- Service above ~400°C: tempering effects degrade the heat-treated structure.
- Ductility-critical snap features: 2-4% elongation as-sintered (<0.5% in HT) — design clips and living hinges from wrought material.
FN-0408 Processing & Heat Treatment
Compaction & Sintering
- Compaction pressure: 600-700 MPa for the 7.1-7.4 g/cm³ window (single press); higher densities via sizing/coining
- Sintering temperature: 1120-1150°C (industry-standard ferrous PM practice is 1120°C, 20-30 minutes at temperature; higher-temperature sintering up to ~1290°C is used for premium metallurgy)
- Atmosphere: endothermic gas or dissociated ammonia/nitrogen-hydrogen, with carbon potential controlled to hold the 0.6-0.9% combined carbon target
- Cooling: controlled cooling rate to prevent thermal cracking and to set the pearlite/bainite balance
Carbon control is the critical FN-0408 process variable: 0.1% combined carbon error moves tensile strength and heat-treat response measurably. Atmosphere dew point and graphite addition accuracy are monitored per lot.
Heat Treatment Options
| Process | Parameters | Result | Use For |
|---|---|---|---|
| Through-hardening (quench + temper) | Austenitize ~840-870°C, oil quench, temper 150-200°C | 40-41 HRC apparent; 860-1000 MPa tensile (density-dependent) | Wear plates, sprockets, high-strength structural |
| Carburizing + quench | Gas carburize in the standard 900-930°C range, quench, temper | 58-62 HRC surface with tough HRB core; effective case 0.5-1.5 mm | Gears needing hard flanks + shock-tolerant core |
| Steam treatment | 510-570°C superheated steam | Fe₃O₄ surface layer; +corrosion resistance, modest hardness gain | Corrosion protection without distortion |
| Sizing/coining | Room-temperature re-press | +0.1-0.3 g/cm³ density; ±0.05 mm tolerance | Precision functional surfaces |
Dimensional change: through-hardening distortion on PM parts is small but real (±0.05-0.15% growth/shrink depending on section and quench severity) — we validate per geometry and adjust green compact dimensions to compensate.
Secondary Operations
Commonly required: sizing/coining, machining of critical features, surface grinding. Optional: shot peening (fatigue life), steam treatment (corrosion), zinc/nickel plating, epoxy or resin vacuum impregnation for pressure-tightness. See our sizing and coining guide for tolerance detail.
FN-0408 Design Guidelines
Tolerances & Surface Finish
- As-sintered: ±0.3% in the press direction, ±0.5% perpendicular; flatness ±0.002"/inch of characteristic length
- After sizing: ±0.05 mm on sized diameters is standard; ±0.025 mm achievable on short features
- Surface finish: Ra 3-8 µm as-sintered; Ra 1.6 µm after tumbling; Ra 0.4-0.8 µm after grinding
Stress & Safety Factors
Working from the as-sintered envelope (yield 380-520 MPa):
- Static loads: design stress ≤50% of yield at the specified minimum density
- Fatigue loads: use 0.3-0.35 × tensile strength as the 10⁷-cycle bending fatigue basis for smooth specimens; apply shot peening or density upgrades when margins are thin
- Shock loads: the nickel-rich austenite phase provides impact tolerance, but validate Charpy/V-notch values at production density — impact energy is the property most sensitive to porosity
Porosity & Section Design
At 90-94% density, interconnected porosity remains (6-10%). Consequences for design:
- Not pressure-tight without resin impregnation
- Avoid knife-edge sections and sharp internal corners (fillets R ≥ 0.8 mm)
- Draft and punch-out relief follow standard PM practice per our DFM guide
FN-0408 vs Alternative Materials
All PM values as-sintered from the same production practice (HT variants noted).
| Material | Density (g/cm³) | Tensile (MPa) | Yield (MPa) | Elongation | Hardness | Relative Cost | Best Fit |
|---|---|---|---|---|---|---|---|
| FN-0408 | 7.1-7.4 | 520-720 | 380-520 | 2-4% | 80-100 HRB | 1.0x (FN family ref.) | Premium gears, extreme-load bearings |
| FN-0405 | 7.1-7.3 | 480-620 | 340-480 | 2-4% | 75-95 HRB | ~0.9x | High-strength gears, slightly better toughness/cost balance |
| FN-0208 | 7.0-7.2 | 450-620 | 300-420 | 2-5% | 70-90 HRB | ~0.8x | Toughness-critical, impact-loaded parts |
| FN-0205 | 6.8-7.1 | 380-480 | 240-340 | 2-5% | 65-85 HRB | ~0.7x | Moderate-duty, cost-sensitive strength |
| FC-0808 | 7.0-7.2 | 420-620 | 280-400 | 1-3% | 70-90 HRB | ~0.6x | Heavy structural without nickel cost |
| FN-0408HT | 6.7-7.1 | 860-1000 | 740-860 | <0.5% | 40-41 HRC | 1.0x + heat treat | Maximum strength, wear-dominated duty |
| Machined medium-carbon steel (1045/4140) | 7.85 (wrought) | 600-1000+ | 350-700+ | 10-25% | HRB 85-HRC 55 | 2-4x at volume | Low volumes, ductility-critical, pressure-tight |
Selection logic:
- Need maximum PM strength and accept heat-treat cost: FN-0408HT
- Need high as-sintered strength with better shock tolerance: FN-0405 (slightly lower strength, better cost)
- Impact-dominated duty: FN-0208
- Strength up, nickel cost down: FC-0808
- Ductility >4% or pressure-tight required: wrought machining — or accept impregnation
For the full decision tree, see FN-0205 vs FN-0405 vs FN-0408.
Case Study: High-Torque Power Tool Planetary Gears (Representative Scenario)
The following is an application scenario representative of FN-0408 power-tool gear programs; figures are typical industry values, not a specific customer's data.
Scenario
A power-tool manufacturer is developing a professional-grade impact driver. The planetary gear set (3 planets, ~35 g each) must transmit 80+ N·m output torque through 3,000+ impacts per minute, with a 50,000-unit annual volume. The incumbent plan is machined 4140 steel, carburized.
Material Options Evaluated
| Factor | Machined 4140 (carburized) | FN-0408 as-sintered | FN-0408HT |
|---|---|---|---|
| Tensile strength | ~900 MPa (core ~750) | 600-650 MPa @ 7.25 g/cm³ | ~900 MPa |
| Tooth surface | HRC 58-62 | 95-100 HRB | HRC 58-60 (carburized core 40 HRC) |
| Impact tolerance | Good | Very good (Ni-austenite phase) | Good (HT core) |
| Unit cost (50K/yr) | Baseline | ~45% lower | ~30% lower |
| Tooling | Moderate | High (gear dies + sizing) | High + heat treat |
| Lead time (ramp) | 8-10 weeks | 4-5 weeks | 5-6 weeks |
| Weight | 100% | ~92% | ~92% |
Outcome Path
Testing showed as-sintered FN-0408 met torque-life targets for consumer-duty use but showed tooth-root wear beyond the professional-duty cycle target; the FN-0408HT (through-hardened) configuration met the full professional duty cycle with margin, at a unit cost well below machined 4140. The program moved forward with FN-0408HT planets plus a sizing operation on the planet carrier bore.
Lesson: FN-0408's as-sintered envelope covers heavy general duty; when duty cycles are extreme, the HT upgrade retains PM's cost advantage over machining while unlocking 860-1000 MPa strength.
Running a similar torque-dense gear program? Send us the duty cycle and gear data — we will recommend density, carbon target, and heat-treat route.
Request FN-0408 Feasibility Review →
Why Choose SinterWorks PM for FN-0408 Components
✅ Premium Ferrous PM Experience
- Manufacturing press-and-sinter components since 2010 — 16 years of FN-family production for automotive, power tool, and industrial customers
- Kia SQ qualified supplier with automotive program discipline on density, carbon, and dimensional control
- National High-Tech Enterprise with patented PM process designs for gear and structural components
✅ FN-0408 Process Control
- Density control across 7.1-7.4 g/cm³ with per-lot verification
- Combined-carbon control (0.6-0.9% C) via atmosphere management — the variable that makes or breaks FN-0408 heat-treat response
- In-house sizing, steam treatment, and heat treatment partners qualified for quench-and-temper and carburizing routes
- Metallurgical validation: apparent hardness, microstructure, and combined-carbon analysis per lot
🎯 Start Your FN-0408 Program
Send drawings, load data, or just the duty cycle. Within 24 hours you receive:
- Material confirmation — FN-0408 vs FN-0405/FN-0208/FC-0808 fit for your loads
- Density + condition recommendation — as-sintered or HT, with the property basis
- Tolerance & secondary-operation plan — sizing, machining, surface treatment
- Cost comparison — PM vs your current route at your volume
Contact: Yao Qingpu, pm@sinterworks-pm.com — response within 24 hours.
Upload Drawing for Free DFM Review →
Frequently Asked Questions
What is the difference between FN-0408 and FN-0205?
FN-0408 carries ~4% nickel and 0.6-0.9% combined carbon versus ~2% nickel and ~0.5% carbon in FN-0205 (both per MPIF Standard 35). In production practice that yields roughly 40-50% higher as-sintered tensile strength (520-720 vs 380-480 MPa), higher hardness (80-100 vs 65-85 HRB), and a stronger quench-and-temper response. FN-0205 remains the better cost choice for moderate loads and impact-critical parts where ultimate strength is not the binding constraint.
What strength can FN-0408 reach after heat treatment?
MPIF Standard 35 tabulates FN-0408HT (quench + temper) at 860 MPa tensile / 40 HRC at 6.7 g/cm³ and 1000 MPa / 41 HRC at 7.1 g/cm³, with yield around 740-860 MPa. Elongation falls below 0.5%, so HT parts are for strength/wear duty, not ductile failure containment. Carburized FN-0408 reaches 58-62 HRC surface with a tougher core.
What density should I specify for FN-0408?
7.1-7.4 g/cm³ is the production window that supports the 520-720 MPa as-sintered envelope. Choose 7.1-7.25 g/cm³ for general structural duty (best cost), 7.3-7.4 g/cm³ for gears and fatigue-loaded parts (pore structure dominates fatigue life). Above ~7.4 g/cm³, double pressing or [copper infiltration](/glossary/infiltration/) becomes the cost-effective route rather than more press tonnage.
Can FN-0408 be used without heat treatment?
Yes — as-sintered FN-0408 at 7.1-7.4 g/cm³ already delivers 520-720 MPa with 2-4% elongation, which covers most structural and moderate-duty gear applications. Heat treatment is justified when surface hardness beyond 100 HRB (wear), or tensile beyond ~720 MPa (extreme load), is required.
Is FN-0408 corrosion resistant?
No. It is a ferrous PM steel with Low-Moderate corrosion resistance. Standard mitigations are steam treatment (Fe₃O₄ barrier), zinc or nickel plating, or oil-coat. For continuously wet or chloride environments, switch to [304 stainless PM](/materials/304-stainless-steel-pm/) or [316L](/materials/316l-stainless-steel-pm/) and accept the strength reduction — or redesign with a plated FN-0408 core where loads dominate.
How does FN-0408 compare to machined medium-carbon steel?
Machined 1045/4140 is stronger in ductility and pressure-tightness (wrought, full density) and needs no tooling — it wins below roughly 5,000-20,000 parts/year depending on complexity. FN-0408 wins at volume: 40-60% unit cost reduction, net-shape tooth forms and blind features that are expensive to machine, and stable per-part economics once tooling is amortized. If maximum ductility or hydraulic pressure-tightness is required, wrought remains the safer specification.
What tolerances can FN-0408 hold?
As-sintered: ±0.3% (press direction) to ±0.5% (perpendicular). After sizing/coining: ±0.05 mm standard, ±0.025 mm on short sized features. Gear programs with dedicated tooling reach GB9/DIN 8 tooth quality. Post-sinter machining is used for features outside these bands — budget it in early so the PM cost advantage survives.
Standards & References
Grade designations and material property data on this page follow published powder metallurgy industry standards. Current editions are available from the publishers:
- MPIF Standard 35 — Materials Standards for PM Structural Parts — Metal Powder Industries Federation (MPIF)
- ASTM International — metal powder and PM material specifications — ASTM International
- ISO 5755 — Sintered metal material: Specifications — ISO
For critical applications, always verify grade data against the current edition of the applicable standard and your part-specific validation requirements.
Expert Review
Yao Qingpu
Powder Metallurgy Manufacturing Expert at SinterWorks PM
Yao Qingpu works with global buyers on powder metallurgy design review, material selection, tolerance planning, cost-down opportunities, and production feasibility. His experience covers PM gears, automotive components, structural parts, and practical DFM support for long-run manufacturing programs.
Related Resources
Use these internal links to keep moving through the most relevant guides, service pages, and technical references for this topic.
FN-0205 Material Guide
Compare FN-0408 with a lower-alloy iron-nickel PM route when strength targets are lower and cost sensitivity is higher.
FN-0405 High-Nickel Alloy
Review another higher-strength PM alloy route when your part needs more fatigue margin or heat-treatment flexibility.
PM Material Grades Overview
See where FN-0408 sits among other iron-nickel PM steel grades in the MPIF Standard 35 overview.
Request a Quote
Send your load case, density target, and annual demand for FN-0408 material review and quotation support.